Rubber Glass Transition
Measurement of the Glass Transition Temperature of Rubber Materials by Differential Scanning Calorimetry (DSC)
The glass transition temperature (Tg) is an important parameter for polymer materials (such as rubber), representing the temperature at which the material transforms from a glassy state to a high-elastic state. This parameter directly affects the low-temperature performance, elastic modulus, and application scenarios of rubber. Differential scanning calorimetry (DSC) is a widely used technique for determining Tg. By measuring the changes in heat flow of a material during heating or cooling, the phase tra...
I. Experimental Principle
A differential scanning calorimeter compares the difference in heat flow between the sample and the reference under programmed temperature control to detect the thermal effects of the material. When rubber undergoes a glass transition, its heat capacity (Cp) changes abruptly, which appears as a step-like baseline shift on the DSC curve (Figure 1). Tg is usually taken as the midpoint or inflection point of this curve shift.

II. Experimental Procedure
1. Sample Preparation
- Sample selection: Take 5–10 mg of rubber sample, avoiding contamination with impurities.
- Pretreatment: If the sample contains plasticizers, fillers, etc., record the composition; if necessary, perform annealing to eliminate thermal history.
- Sealing: Place the sample in an aluminum crucible, press and seal tightly. The reference should be an empty crucible or inert material (such as alumina).
2. Equipment Selection
- Instrument: DSC600 Differential Scanning Calorimeter.
- Instrument parameter settings:
- Temperature range: generally set from -100 ℃ to 50 ℃ (adjust according to the type of rubber).
- Heating rate: recommended 10–20 ℃/min (too fast may cause Tg shift).
- Atmosphere control: nitrogen atmosphere (flow rate 50–100 mL/min) to prevent oxidation reactions.
- Baseline calibration: calibrate the instrument with standard substances (such as indium, tin).
3. Test Process
- Baseline test with an empty crucible.
- Insert the sample and run a heating–cooling–heating cycle (to eliminate thermal history).
- Record the second heating curve for Tg analysis.
4. Reference Standards
- GB/T 19466.2-2004 / ISO11357-2:1999 Plastics — Differential Scanning Calorimetry — Part 2: Determination of Glass Transition Temperature.
- GB/T 29611-2013 Raw Rubber — Determination of Glass Transition Temperature by DSC.
III. Data Analysis
- Tg determination: On the DSC curve, the glass transition appears as a step-like change. According to GB/T19466.2-2004 / ISO11357-2:1999, Tg is taken as the temperature at the midpoint of the baseline shift.
- Software processing: Use the instrument’s software to perform tangent analysis to determine the onset, midpoint, and endpoint.
Factors affecting the measurement results:
1. Heating rate: Too fast a rate may cause Tg to shift toward higher temperatures; 10 ℃/min is recommended.
2. Sample homogeneity: Uneven distribution of fillers or plasticizers may lead to multiple transition peaks.
3. Elimination of thermal history: The first heating must cover temperatures above the melting point of the material, then cool to low temperatures to erase processing history.
4. Moisture interference: Hygroscopic rubbers should be pre-dried to avoid endothermic peaks from evaporation masking Tg.
Practical application examples:
- Natural rubber (NR): Typical Tg about -70 ℃ to -60 ℃.
- Styrene-butadiene rubber (SBR): Tg ranges from -50 ℃ to -30 ℃, influenced by styrene content.
- Fluoroelastomer (FKM): Higher Tg (about -20 ℃ to 0 ℃), so the test range needs to be adjusted to -50 ℃ ~ 100 ℃.
Conclusion:
Differential scanning calorimetry is a reliable method for determining the Tg of rubber. Accurate measurement provides essential data for rubber formulation design, quality control, and evaluation of low-temperature performance.